Performances du Procédé
| Matériaux | Type |
Durée de vie |
Energie de surface (mN/m²) | |
| Avant | Après | |||
| Polyoléfines | PP | 60 | 32 | 66 |
| PE | 60 | 30 | 66 | |
|
Thermoplastiques Standards |
PS | 30 | 32 |
64 |
| PA 6.6 |
30 | 42 | 68 | |
| PA 6 |
30 | 42 | 68 | |
| PET | 60 | 37 | 58 | |
| PMMA | 15 | 40 | > 72 |
|
| PCTA | 15 | 42 | 67 | |
| PETG | 15 | 39 | 70 | |
| Plastiques techniques |
POM | 10 |
38 |
50 |
| PEI | 30 | 40 | 66 | |
| PBT | 60 | 42 | > 72 | |
| Phéno. | 15 | 45 | > 72 | |
| PI | 15 | 42 | 54 |
|
| PEEK | 15 | 38 | 54 | |
| PC | 15 | 38 | > 72 |
|
| PVDF | 10 | 32 | 50 | |
| Vernis UV |
UV |
15 |
35 |
58 |
| Copolymères | ABS |
10 |
40 |
64 |
| Composites & alliages |
ABS/PC | 5 |
40 |
64 |
| PBT/FV |
60 | 42 | > 72 | |
| Elastomères | SiF | 1 | 28 | 46 |
| SiO2 | 1 | 46 | > 72 | |
| EPDM | 15 | 44 | 67 | |
| Verre inorganique |
Verre |
< 1 |
46 |
> 72 |
| Métaux | Zamac | 7 |
50 | > 72 |
| Al | 7 | 50 | > 72 | |
| CuBe | 7 | 41 | 65 | |
| Acier C |
4 | 47 |
70 |
|
| Acier13Cr | 4 | 33 | 70 | |
| Autres | nous consulter | |||
La durée de vie est le temps maximal de conservation du traitement avant application à partir duquel une diminution sensible des performances est constatée .
L’énergie de surface est mesurée par la méthode de Owens-Wendt sur un banc de mesure d’angle de contact doté d’un système d’analyse d’image. Les valeurs données correspondent à une moyenne de l’énergie totale (dispersive+polaire). Les liquides utilisés sont l’eau, le formamide, le dimétylsulfone et la pyridine.